Heat Resistance
TPX™ has a high melting point in the range from 220°C to 240°C and a high vicat softening temperature. Hence, it can be used for high temperature application. However, as heat distortion temperature of TPX™ is almost the same as that of polypropylene, the application under high - stress environment needs to be carefully considered.
Releasability and Non - compatibility
The surface tension of TPX™ (24mN/m) is very low and this value is the second lowest as compared to fluorine polymers. Hereby, TPX™ shows excellent releasability against various materials in hardening process of thermosetting resins (urethane, epoxy etc.). Furthermore, since TPX™ shows incompatibility against thermoplastic resins (PET, PP etc.), it is used to create a porous structure in PET or membranes. Transparency
Although TPX™ is a crystalline polymer, it exhibits excellent transparency (Haze < 5%) and light transmittance. In particular TPX™ is used for optical analysis cells because of the higher UV transmittance as compared to glass and other transparent polymers.
TPX™ applications include:
List | Methodology | Measured Condition / Sample Condition | Unit | RT18 (RT18BK) | RT31 (RT31BK) | DX845 |
---|---|---|---|---|---|---|
Density | MCI Method | Density Gradient Method / Pellets | kg/m³ | 833 | 833 | 833 |
MFR | MCI Method | Applied Force = 5kgf, 260 °C / Pellets | g/10 min | 26 | 21 | 9 |
Melting Point | MCI Method | DSC Method / Pellets | °C | 232 | 232 | 232 |
Water Absorption | ISO 62 | Test Piece: 1mm thick | ≤0.01 | ≤0.01 | ≤0.01 | |
Vicat Softening | ISO 306 | Heat Speed: 50°C/h / Test Piece (4mm) | °C | 167 | 167 | 167 |
Heat Distortion Temperature | ISO 75 | Heat Speed: 120°C/hour Applied Stress: 0.45MPa / Test Piece (4mm) | °C | 86 | 90 | 93 |
Linear Expansion | ISO 11359 - 1 | Heat Speed 5°C/min / Test Piece (4mm) | 10/°C | 1.31 | - | 1.72 |
Yield Stress | Cross Head Speed: 5mm/min / Test Piece (4mm) | MPa | 23 | 24 | 24 | |
Cross Head Speed: 50mm/min / Test Piece (4mm) | MPa | 28 | 29 | 28 | ||
Fractured Stress | ISO527 | Cross Head Speed: 5mm/min / Test Piece (4mm) | MPa | 15 | 17 | 16 |
Cross Head Speed: 50mm/min / Test Piece (4mm) | MPa | - | - | - | ||
Fractured Strain | Cross Head Speed: 5mm/min / Test Piece (4mm) | % | 67 | 60 | 83 | |
Cross Head Speed: 50mm/min / Test Piece (4mm) | % | 32 | 27 | 29 | ||
Tensile Modulus | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 1350 | 1350 | 1480 | |
Flexural Modulus | ISO178 | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 1530 | 1530 | 1520 |
Flexural Strength | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 37 | 40 | 40 | |
Izod Impact Strength | ISO180 | Injection Molded Specimen (Part MCI Method) | kJ/m² | 2 | 2 | 3 |
Injection Molded Specimen (w/o MCI Method) / Test Piece (4mm) | kJ/m² | 7 | 6 | 7 | ||
Rockwell Hardness | ISO2039 | HRR Scale | - | 80 | 78 | |
Haze | ISO14782 | Light Source: D65 / Test Piece(2mm thick) | % | 2.4 | 2.4 | 2.8 |
Internal Haze | Light Source: D65 / Test Piece(2mm thick) | % | 93.0 | 93.0 | 93.0 | |
Refractive Index | ISO489 | Light Source: D Line / Test Piece(2mm thick) | 1.462 | 1.462 | 1.463 | |
Volume Resistivity | IEC60093 | Injection Molded Specimen (2mm thick) | Ω·cm | >10¹5 | >10¹5 | >10¹5 |
Breakdown Voltage | IEC60243 - 1 | Injection Molded Specimen (2mm thick) | kV/mm | 30 | 29 | 29 |
Relative Dielectric | IEC60250 | 1MHz / Injection Molded Specimen (2mm thick) | 2.15 | 2.12 | 2.16 | |
Spiral Flow | MCI Method | 310°C~320°C, Mold Temperature: 73°C | cm | 51 | 51 | 50 |
Mold Shrinkage | MCI Method | Injection Molded Specimen (2mm thick) TD | % | 1.6 | 1.6 | 1.5 |
Injection Molded Specimen (2mm thick) MD | % | 1.3 | 1.3 | 1.4 |
List | Methodology | Measured Condition / Sample Condition | Unit | DX820 | DX231 | MX004 | DX324 | MX002 | MX002O | MX001 |
---|---|---|---|---|---|---|---|---|---|---|
Density | MCI Method | Density Gradient Method / Pellets | kg/m³ | 832 | 832 | 833 | 833 | 834 | 834 | 834 |
MFR | MCI Method | Applied Force = 5kgf, 260 °C / Pellets | g/10 min | 180 | 100 | 25 | 25 | 21 | 21 | 27 |
Melting Point | MCI Method | DSC Method / Pellets | °C | 233 | 232 | 228 | 227 | 224 | 224 | 223 |
Water Absorption | ISO 62 | Test Piece: 1mm thick | 0.01 | 0.01 | ≤0.01 | 0.01 | ≤0.01 | ≤0.01 | 0.01 | |
Vicat Softening | ISO 306 | Heat Speed: 50°C/h / Test Piece (4mm) | °C | 171 | 179 | 161 | 162 | 151 | 149 | 147 |
Heat Distortion Temperature | ISO 75 | Heat Speed: 120°C/hour Applied Stress: 0.45MPa / Test Piece (4mm) | °C | 86 | 90 | 80 | 79 | 74 | 72 | 72 |
Linear Expansion | ISO 11359 - 1 | Heat Speed 5°C/min / Test Piece (4mm) | 10-5/°C | 1.03 | - | 1.44 | - | 1.53 | - | - |
Yield Stress | Cross Head Speed: 5mm/min / Test Piece (4mm) | MPa | - | 26 | 18 | 19 | 14 | 14 | 14 | |
Cross Head Speed: 50mm/min / Test Piece (4mm) | MPa | 25 | 28 | 23 | 22 | 18 | 18 | 18 | ||
Fractured Stress | ISO527 | Cross Head Speed: 5mm/min / Test Piece (4mm) | MPa | 25 | 26 | 12 | 13 | 12 | 11 | 12 |
Cross Head Speed: 50mm/min / Test Piece (4mm) | MPa | 29 | 31 | - | - | 10 | 11 | 11 | ||
Fractured Strain | Cross Head Speed: 5mm/min / Test Piece (4mm) | % | 3 | 5 | 155 | 80 | 226 | 189 | 211 | |
Cross Head Speed: 50mm/min / Test Piece (4mm) | % | 3 | 5 | 29 | 31 | 37 | 45 | 46 | ||
Tensile Modulus | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 1630 | 1490 | 770 | 690 | 430 | 510 | 490 | |
Flexural Modulus | ISO178 | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 1600 | 1550 | 810 | 750 | 530 | 540 | 530 |
Flexural Strength | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 43 | 41 | 26 | 24 | 18 | 19 | 19 | |
Izod Impact Strength | ISO180 | Injection Molded Specimen (Part MCI Method) | kJ/m² | 2 | 1 | 1 | 1 | 2 | 3 | 2 |
Injection Molded Specimen (w/o MCI Method) / Test Piece (4mm) | kJ/m² | 6 | 6 | 14 | 23 | NB | NB | NB | ||
Rockwell Hardness | ISO2039 | HRR Scale | 94 | 90 | 59 | 55 | 29 | 38 | 37 | |
Haze | ISO14782 | Light Source: D65 / Test Piece(2mm thick) | % | 3.7 | 3.6 | 2.5 | 2.3 | 2.3 | 1.6 | 1.8 |
Internal Haze | Light Source: D65 / Test Piece(2mm thick) | % | 92.0 | 92.0 | 93.0 | 92.0 | 92.0 | 93.0 | 92.0 | |
Refractive Index | ISO489 | Light Source: D Line / Test Piece(2mm thick) | 1.462 | 1.462 | 1.463 | 1.463 | 1.463 | 1.463 | 1.463 | |
Volume Resistivity | IEC60093 | Injection Molded Specimen (2mm thick) | Ω·cm | >10¹5 | >10¹5 | >10¹5 | >10¹5 | >10¹5 | >10¹5 | >10¹5 |
Breakdown Voltage | IEC60243 - 1 | Injection Molded Specimen (2mm thick) | kV/mm | 31 | 31 | 30 | 28 | 29 | 29 | 29 |
Relative Dielectric | IEC60250 | 1MHz / Injection Molded Specimen (2mm thick) | 2.13 | 2.12 | 2.17 | 2.13 | 2.19 | 2.12 | 2.12 | |
Spiral Flow | MCI Method | 310°C~320°C, Mold Temperature: 73°C | cm | - | - | 53 | - | 56 | 56 | - |
Mold Shrinkage | MCI Method | Injection Molded Specimen (2mm thick) TD | % | - | - | 1.7 | - | 1.6 | 1.6 | - |
Injection Molded Specimen (2mm thick) MD | % | - | - | 1.4 | - | 1.3 | 1.3 | - |
List | Methodology | Measured Condition / Sample Condition | Unit | DX310 | DX820M | DX560M | MLL411 | MB2230(A) |
---|---|---|---|---|---|---|---|---|
Density | MCI Method | Density Gradient Method / Pellets | kg/m³ | 834 | 840 | 856 | 834 | 1100 |
MFR | MCI Method | Applied Force = 5kgf, 260 °C / Pellets | g/10 min | 100 | 220 | 33 | 20 | 57 |
Melting Point | MCI Method | DSC Method / Pellets | °C | 224 | 233 | 222 | 222 | 232 |
Water Absorption | ISO 62 | Test Piece: 1mm thick | ≤0.01 | 0.04 | ≤0.01 | 0.05 | ||
Vicat Softening | ISO 306 | Heat Speed: 50°C/h / Test Piece (4mm) | °C | 144 | 140 | 87 | 141 | 169 |
Heat Distortion Temperature | ISO 75 | Heat Speed: 120°C/hour Applied Stress: 0.45MPa / Test Piece (4mm) | °C | 75 | 85 | 53 | 69 | 91 |
Yield Stress | Cross Head Speed: 5mm/min / Test Piece (4mm) | MPa | 15 | - | 7 | 9 | 22 | |
Cross Head Speed: 50mm/min / Test Piece (4mm) | MPa | 18 | - | 7 | 12 | 26 | ||
Fractured Stress | ISO527 | Cross Head Speed: 5mm/min / Test Piece (4mm) | MPa | 11 | 23 | 8 | 11 | - |
Cross Head Speed: 50mm/min / Test Piece (4mm) | MPa | 10 | 27 | 8 | 12 | - | ||
Fractured Strain | Cross Head Speed: 5mm/min / Test Piece (4mm) | % | 230 | 3 | 319 | 221 | 29 | |
Cross Head Speed: 50mm/min / Test Piece (4mm) | % | 38 | 3 | 238 | 166 | 21 | ||
Tensile Modulus | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 520 | 1390 | 170 | 250 | 1720 | |
Flexural Modulus | ISO178 | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 550 | 1450 | 190 | 250 | 1910 |
Flexural Strength | Cross Head Speed: 1mm/min / Test Piece (4mm) | MPa | 20 | 38 | 6 | 10 | 41 | |
Izod Impact Strength | ISO180 | Injection Molded Specimen (Part MCI Method) | kJ/m² | 1 | 1 | NB | NB | 9 |
Injection Molded Specimen (w/o MCI Method) / Test Piece (4mm) | kJ/m² | 24 | 7 | NB | NB | 30 | ||
Rockwell Hardness | ISO2039 | HRR Scale | 45 | 84 | - | - | 73 | |
Haze | ISO14782 | Light Source: D65 / Test Piece(2mm thick) | % | 2.2 | - | - | - | - |
Internal Haze | Light Source: D65 / Test Piece(2mm thick) | % | 92.0 | - | - | - | - | |
Volume Resistivity | IEC60093 | Injection Molded Specimen (2mm thick) | Ω·cm | >10¹5 | >10¹5 | >10¹5 | >10¹5 | >10¹5 |
Breakdown Voltage | IEC60243 - 1 | Injection Molded Specimen (2mm thick) | kV/mm | 28 | 30 | 31 | 29 |
Packaging:
Transportation:
Handling Precautions:
Contact Us: Get in touch to start our collaboration today.
Q1. Are you a factory or trading company?
Q2. Can I get samples for testing?
A: Yes, we provide samples. Customers cover the initial shipping costs, which are reimbursed in our first cooperation.
Q3. How does your factory ensure quality control?
A: Our factory is ISO9001:2008, REACH, and FAMIQS certified, ensuring rigorous quality control. Each Batch of goods do SGS inspection before leaving our factory.
Q4. What's your Delivery Time?
A: Delivery typically takes 5 to 10 days after payment receipt. Larger orders are confirmed with our production department for prompt, quality-assured delivery.
Q5. What are your payment terms?
A: We accept L/C, T/T, Western Union, and Paypal. Alternative methods can be discussed.
Q6. Which documents do you provide?
A: Standard documents include Commercial Invoice, Price List, Packing List, COA, Origin Certificate, Quality/Quantity Certificate, Beneficiary's Certificate, MSDS, B/L, and others upon request.
Additional Information: